Jun 06, 2023
「希土類含有量が最も低い場合、薄壁の内面に厚さ約 0.2-0.6 mm の片状黒鉛層が形成されることがあります。これは強度に本質的な影響を与えません」キャスティングの。」 寿港鋳造所で4.5トンのマス鋼鋳鉄インゴットモールドを製造したところ、厚さ2.5トンのインク層があることが判明した。<1.5 mm on its outer surface. The existence of the ink layer is unfavorable to the castings subjected to fatigue load. The formation of the ink layer is mainly the result of the interaction between the molten iron and the surface of the mold and core. Since the Su and type materials themselves contain a certain amount of sulfur, during their drying process, part of the sulfide produced by fuel combustion will also be adsorbed on the surface of the type and core, and these sulfur will consume magnesium, cerium, calcium, etc. on the surface of the molten iron. The content of the element is greatly reduced, or it is related to "the oxidation of the surface of the casting, which greatly reduces the content of rare earth (1/3-1/2 times)", and it is believed that nitrogen in addition to sulfur and oxygen will also produce a sheet ink layer. The formation of the ink layer is the result of the comprehensive action of sulfur, oxygen and nitrogen.
インクのフレークの形成を防ぐために、Jianzhi Magang では、成形品、コア材料、コーティング、燃料中の硫黄含有量を可能な限り低く保つ必要があります。 同時に、溶融鉄にチタンとセリウムをさらに追加すると、この種の欠陥を効果的に克服できます。
建治可鍛鋼による型固着の直接の原因は、鋳物砂の強度が低すぎること、つまり、砂粒間の付着力がパターン上の砂粒の付着力よりも小さいことです。 具体的な理由は次のとおりです。
1. 注湯ライザーシステム
ゲートライザーシステムの設計は、通常、粘着性のある多肉植物の欠陥の発生にはほとんど影響しません。
2. 鋳物砂
(1)鋳物砂が過熱される。 ホットサンドは脆くなり、せん断力を受けると簡単に壊れる傾向があります。
(2) 鋳物砂の性能は不適格です。 通常、鋳物砂の配合は、水が多すぎる、砂の混合が不均一である、補助材料が多すぎるなど、不適格です。
3. 中子作り
中子箱内でベタベタした砂中子は型に入れることができません。 砂中子のバインダーと離型剤が化学反応を起こした場合も、カビのベタつきの原因となります。 湿式中子とは、成形時に型から成形され、型抜き後に砂型から取り出される砂中子を指します。 一般的に上型の場合は吊り砂と呼ばれ、上型は吊り砂と呼ばれます。 下のタイプでは、タップサンドコアと呼ばれます。 一部の薄肉鋼鋳物では、中子ボックスを使用して湿った砂中子を作成し、乾燥せずに砂型に入れます。 これはまさに湿った砂のコアです。 狭くて高く垂れ下がった砂や水道砂のコアは、粘着性のあるカビや多肉植物が発生しやすいです。 特に機械成形、成形機、生産ペースが速い場合、濡れた砂中子が形状によって固着するという悪い状況を見つけるのは困難です。 逆に手作業での成型や成型に比べてベタベタしたカビや肉付きの欠陥が発生しやすくなります。 この欠陥は湿式鋳造鋳物で発生します。